AISI P20+NI STEEL

AISI P20+NI STEEL


STANDARDS : 40CRMNNIMO8-6-4

AISI P20+Ni

P20+Ni DIN 2738  
C 0.42

Mn 1.50

Cr 1.95

Ni 1.10

Mo 0.20

 

AISI P20+Ni is specially used for Plastic injection die moulds. The characteristics of a material are right sharpening, photo-etching properties with high purity and good homogeneity. AISI P20+Ni is upgraded version of plastic mold steel 0f 2311, which normally supply in Pre hardened condition. Hardness in as supplied condition 280-320 HB with having uniform hardness. The additional nickel content of 1 % increases through hardening. It has good machinability, suitable for Texturing, fine polishability, adequate corrosion resistance, vacuum-degassed steel.

 

AISI P20+Ni High Hard ( HXM 24 )
 

AISI P20+Ni is with High Hardness 360-400 BHN and increase alloy elements to get extra life and outstanding polishing.


Steel Properties

AISI P20 +Ni is upgrade version of plastic mold steel 0f 2311, which normally supply in Pre hardened condition. Hardness in as supplied condition 280-320 HB. The additional nickel content of 1 % increases through hardening. It is micro-alloyed. It has good machinability, suitable for texturing, outstanding polishability, adequate corrosion resistance. vacuum-degassed steel with the following excellent features.

 

Physical Properties

Coefficient of thermal expansionat °C

20-100

20-200

20-300

20-400

20-500

20-600

20-700

10-6 m/(m*K)

11.2

12.8

13.5

13.7

14.3

14.7

14.9

 

Thermal Conductivity at °C

20

350

700

W/(m*K)

35

34

33


Application

AISI P20+Ni is the equivalent grade of DIN 2738 which is applicable for large & small plastic mould dies for Automotive Industries, mould for bumpers, crates, plastic furniture, dashboard, Television cabinets, Boaster Plates of Presses, Die Holders & Shoe blocks for drop Hammers, Press Cassettes , Upsetter Blocker, forging dies, Different dies & mold for plastic products etc.

 

Heat Treatment

Soft annealing °C

Cooling

Hardness HB

710 – 740

Furnace

max. 235

 

Hardening °C

Quenching

Hardness after quenching HRC

840 – 870

Polymer or oil

51

 

Tempering °C after Quenching

100

200

300

400

500

600

700

HRC 51.5 50.2 48 46.2 43 39 29